ASTM A334 Grade 6 Tubes | ASME SA334 Gr 6 Low Temperature Carbon Steel Tubes Supplier & Exporter
ASTM A334 Grade 6 tubes (also ordered as ASME SA334 Gr 6) are seamless and welded carbon steel tubes made for service at sub-zero temperatures. Grade 6 is the most widely specified grade in the A334 standard: a silicon-killed, fine-grained carbon-manganese steel that is Charpy impact tested at -45°C (-50°F) and offers higher strength than Grade 1.
ASC LLP, Mumbai, has supplied low temperature carbon steel (LTCS) tubes since 1984 to refineries, LNG and gas-processing plants, heat-exchanger fabricators and EPC contractors across the USA, Europe, the Middle East and South America.
What Are ASTM A334 Grade 6 Tubes?
ASTM A334/A334M is the standard specification for seamless and welded carbon and alloy-steel tubes for low-temperature service. Unlike pipe standards such as ASTM A333, A334 covers minimum-wall tubes ordered by outside diameter and minimum wall thickness – the format used for heat exchangers, condensers, instrument lines and small-bore process tubing.
Grade 6 (UNS K03006) is a plain carbon-manganese grade with a maximum of 0.30% carbon, 0.29–1.06% manganese and a minimum of 0.10% silicon. The silicon requirement makes it a fully killed steel, and normalizing gives it a fine-grained microstructure. The result is a tube with 415 MPa minimum tensile strength, 240 MPa minimum yield and dependable notch toughness down to -45°C. It is commonly supplied as:
- ASTM A334 Grade 6 Seamless Tubes
- ASME SA334 Gr 6 Welded / ERW Tubes
- A334 Grade 6 Heat Exchanger Tubes
- A334 Gr 6 U-Bend Tubes
- LTCS A334 Grade 6 Cold Drawn Seamless (CDS) Tubes
Types of A334 Grade 6 Tubes We Supply
We supply A334 Grade 6 low temperature tubes in the forms most used by fabricators and EPC buyers:
A334 Grade 6 Seamless Tubes
- Hot finished or cold drawn
- First choice for high-pressure, pressure-rated and critical heat-exchanger duty
SA334 Gr 6 Welded / ERW Tubes
- Welded without filler metal, as the specification requires
- Impact tested across the weld as well as the base metal
- Economical option for many standard applications
A334 Grade 6 Heat Exchanger & Condenser Tubes
- Straight lengths cut to tube-sheet requirements
- Tight OD and wall tolerances per ASTM A1016 for consistent tube-to-tubesheet joints
A334 Gr 6 U-Bend Tubes
- Bent to drawing, with stress relieving of the bend zone when specified
- Hydro tested after bending on request
A334 Grade 6 Instrumentation & Small-Bore Tubes
- Small OD tubes and coils for sampling and instrument lines in cold service
A334 Gr 6 Tubes with NACE MR0175 / HIC Testing
- For sour and hydrogen service, supplied with the required hardness and HIC/SSC test reports

Seamless vs Welded A334 Grade 6 Tubes
A334 Grade 6 Seamless Tubes
- No weld seam – uniform properties around the circumference
- Preferred for high pressure, cyclic and critical service
- Flare test applies
A334 Grade 6 Welded Tubes
- Lower cost and tight wall tolerance
- Charpy specimens taken across the weld as well as from the base metal
- Flange and reverse flattening tests apply
Choose the type based on design pressure, your project specification and budget.
A334 Grade 6 Tubes Quality Control & Testing
Every lot of ASTM A334 Grade 6 tubes is tested to the specification and documented on the mill test certificate:
- Chemical (heat and product) analysis
- Tension test
- Flattening test
- Flare test (seamless) / flange and reverse flattening tests (welded)
- Hardness test (Rockwell / Brinell)
- Charpy V-notch impact test at -45°C
- Hydrostatic test or non-destructive electric test (eddy current / ultrasonic) per ASTM A1016
- Visual and dimensional inspection
- Optional: PMI, HIC, NACE MR0175 / MR0103, third-party inspection (TÜV, BV, SGS, Lloyd’s, DNV)
Tubes are marked with specification, grade, size, heat number, manufacturer and the letters “LT” followed by the impact test temperature (e.g. LT-50), as required by A334.


Specifications Table – ASTM A334 Grade 6 Tubes
| Parameter | Details |
| Standard | ASTM A334 / A334M, ASME SA334 / SA334M |
| Grade | Grade 6 (Gr. 6), UNS K03006 – carbon steel, low temperature service |
| General Requirements | ASTM A1016 / A1016M |
| Type | Seamless (hot finished / cold drawn), Welded (ERW) |
| Outside Diameter | 6.35 mm (1/4″) to 168.3 mm (6″) – other sizes on request |
| Wall Thickness | 0.89 mm to 12.7 mm (minimum wall) |
| Length | Single random, double random, fixed lengths up to 12 m; U-bent tubes to drawing |
| Impact Test Temperature | -45°C (-50°F); lower temperatures on request |
| Heat Treatment | Normalized, normalized & tempered, or controlled hot-finished (seamless) |
| Ends | Plain end, bevelled end, square cut |
| Surface | Black / varnished, anti-rust oil, end caps |
| Test Certification | EN 10204 3.1; 3.2 with third-party inspection on request |
Chemical Composition Table – ASTM A334 Grade 6
| Element | Percentage (%) |
| Carbon (C) | 0.30 max |
| Manganese (Mn) | 0.29 – 1.06 |
| Phosphorus (P) | 0.025 max |
| Sulfur (S) | 0.025 max |
| Silicon (Si) | 0.10 min |
| Iron (Fe) | Balance |
For each reduction of 0.01% carbon below 0.30%, an increase of 0.05% manganese above 1.06% is permitted, up to a maximum of 1.35% Mn. The 0.10% minimum silicon makes Grade 6 a fully killed steel – the key chemical difference from Grade 1.
Mechanical Properties of ASTM A334 Grade 6 Tubes
| Property | Requirement |
| Tensile Strength, min | 60 ksi (415 MPa) |
| Yield Strength, min | 35 ksi (240 MPa) |
| Elongation in 2 in. (50 mm), min – longitudinal | 30% (walls 8 mm / 5/16″ and over) |
| Elongation in 2 in. (50 mm), min – transverse | 16.5% |
| Hardness, max | Rockwell B90 / 190 HB |
| Charpy Impact Test Temperature | -45°C (-50°F) |
Minimum Elongation by Wall Thickness – A334 Grade 6 (Strip Specimens)
| Wall Thickness | Min. Elongation in 2 in. (50 mm) |
| 5/16″ (8 mm) | 30% |
| 9/32″ (7.2 mm) | 28% |
| 1/4″ (6.4 mm) | 27% |
| 7/32″ (5.6 mm) | 26% |
| 3/16″ (4.8 mm) | 24% |
| 5/32″ (4 mm) | 22% |
| 1/8″ (3.2 mm) | 21% |
| 3/32″ (2.4 mm) | 20% |
| 1/16″ (1.6 mm) | 18% |
Values are for longitudinal strip specimens: 1.50 percentage points are deducted from the basic 30% for each 1/32″ (0.8 mm) decrease in wall thickness below 5/16″.
Impact Test Requirements for A334 Grade 6 Tubes (Charpy V-Notch at -45°C)
Impact testing is what makes A334 Grade 6 a low temperature tube. Charpy V-notch specimens are tested to ASTM E23 at -45°C. Because tube walls are often too thin for full-size specimens, A334 allows sub-size specimens with proportionally lower energy values. For welded tubes, specimens are taken from the weld as well as the base metal.
Charpy Impact Requirements – A334 Grade 6
| Specimen Size (mm) | Min. Average of 3 Specimens | Min. for One Specimen |
| 10 × 10 (full size) | 13 ft·lbf (18 J) | 10 ft·lbf (14 J) |
| 10 × 7.5 | 10 ft·lbf (14 J) | 8 ft·lbf (11 J) |
| 10 × 6.67 | 9 ft·lbf (12 J) | 7 ft·lbf (9 J) |
| 10 × 5 | 7 ft·lbf (9 J) | 5 ft·lbf (7 J) |
| 10 × 3.33 | 5 ft·lbf (7 J) | 3 ft·lbf (4 J) |
| 10 × 2.5 | 4 ft·lbf (5 J) | 3 ft·lbf (4 J) |
Important for buyers: when the sub-size specimen width along the notch is less than 80% of the actual wall thickness, the test temperature must be lowered below -45°C by the amount set out in the specification. Very small tubes that cannot yield even the smallest sub-size specimen are exempt from impact testing. If your design needs toughness below -45°C, state the lower test temperature on the purchase order.
ASTM A334 Grades and Their Impact Test Temperatures
| A334 Grade | Type | Impact Test Temperature |
| Grade 1 | Carbon steel | -45°C (-50°F) |
| Grade 6 | Carbon steel (Si-killed) | -45°C (-50°F) |
| Grade 7 | 2.5% nickel steel | -75°C (-100°F) |
| Grade 9 | Nickel-copper steel | -75°C (-100°F) |
| Grade 3 | 3.5% nickel steel | -100°C (-150°F) |
| Grade 8 | 9% nickel steel | -195°C (-320°F) |
Grade 6 is the standard carbon steel choice down to -45°C. For colder service, move up to a nickel-bearing grade.
Heat Treatment of ASTM A334 Grade 6 Tubes
All Grade 6 tubes must be treated to control their microstructure by one of these methods:
- Normalizing – heating to a uniform temperature of not less than 845°C (1550°F) and cooling in air or in the cooling chamber of an atmosphere-controlled furnace.
- Normalizing and tempering – normalized as above and, at the manufacturer’s discretion, reheated to a suitable tempering temperature.
- Controlled hot finishing (seamless only) – hot working finished between 845–955°C (1550–1750°F) and cooled in a controlled-atmosphere furnace from not less than 845°C.
ASTM A334 Grade 6 vs Grade 1 vs A333 Grade 6
| Feature | A334 Grade 6 | A334 Grade 1 | A333 Grade 6 |
| Product Form | Tube (OD × min wall) | Tube (OD × min wall) | Pipe (NPS × schedule) |
| Carbon, max | 0.30% | 0.30% | 0.30% |
| Manganese | 0.29–1.06% | 0.40–1.06% | 0.29–1.06% |
| Silicon | 0.10% min | No requirement | 0.10% min |
| Tensile, min | 415 MPa | 380 MPa | 415 MPa |
| Yield, min | 240 MPa | 205 MPa | 240 MPa |
| Hardness, max | B90 / 190 HB | B85 / 163 HB | — |
| Impact Test Temp. | -45°C | -45°C | -45°C |
Which should you choose? Grade 6 and Grade 1 share the same -45°C impact temperature. Grade 6 is killed with silicon and is about 35 MPa stronger in both tensile and yield, so it is the usual choice for pressure-rated exchangers and process tubing, and it pairs with A333 Grade 6 pipe in the same LTCS piping class. Grade 1 is softer (B85 max), which can help with heavy roller expansion or very tight U-bends – see our ASTM A334 Grade 1 Tubes. For pipe sizes by schedule, see our ASTM A333 Gr 6 Low Temperature Pipes.
ASTM A334 Grade 6 Equivalent Grades
| Standard | Equivalent Grade |
| ASTM | A334 Grade 6 |
| ASME | SA334 Grade 6 |
| UNS | K03006 |
| EN (nearest) | P265NL – EN 10216-4 / EN 10217-4 |
| JIS (nearest) | STBL 380 – JIS G3464 |
| DIN (legacy) | TTSt 35 N (1.0356) |
Equivalents are approximate. Impact test temperatures and energy values differ between ASTM and EN standards – confirm suitability against your design code before substituting.
How to Order ASTM A334 Grade 6 Tubes
To get an accurate quote quickly, include these details in your enquiry:
- Quantity (metres, number of lengths or tonnes)
- Specification and grade – ASTM A334 / ASME SA334 Grade 6
- Seamless or welded
- Outside diameter and minimum wall thickness
- Length – random, fixed cut, or U-bend drawing
- Impact test temperature if lower than -45°C
- Optional requirements – NACE / HIC, PMI, NDE method, third-party inspection
- Certification – EN 10204 3.1 or 3.2
Applications of ASTM A334 Grade 6 Tubes
Thanks to their strength and proven toughness at -45°C, A334 Grade 6 low temperature tubes are widely used in:
- Heat exchangers and condensers handling chilled or refrigerated process fluids
- LNG, LPG, NGL and gas-processing plants
- Refrigeration and ammonia plants
- Petrochemical and refinery units – ethylene, propylene, depropanizer and blowdown services
- Air separation units and cold boxes (carbon steel sections above -45°C)
- Offshore and arctic installations
- Instrument and sampling lines in cold climates
Why Choose Us as Your ASTM A334 Grade 6 Tubes Supplier?
With four decades of experience in carbon and low temperature steel tubulars, we understand what project buyers need:
- Since 1984: a long record of supplying carbon, alloy and LTCS tubes
- Mill-sourced material from approved Indian and international seamless tube mills
- Full traceability: heat-wise bundling, stencilled marking, EN 10204 3.1/3.2 MTCs
- Third-party inspection welcomed at the mill and at our Mumbai facility
- Matched LTCS packages: A334 Gr 6 tubes alongside A333 Gr 6 pipes for the same project
- Export-ready packing: hexagonal bundles with steel straps, end caps, wooden boxes for U-tubes
ASTM A334 Grade 6 tubes are the standard choice wherever carbon steel tubing must stay strong and tough below zero. As an experienced A334 Grade 6 tubes supplier and exporter, we focus on correct material, complete documentation and on-time delivery with every order.
Related Products
- ASTM A334 Grade 1 Tubes – softer LTCS tubes, also impact tested at -45°C
- ASTM A333 Grade 6 Pipes – low temperature carbon steel pipes by NPS and schedule
- ASTM A334 / SA334 Carbon Steel Pipes – all A334 grades in one place
- SA179 Seamless Tubes – cold-drawn heat exchanger tubes for normal temperatures
- ASTM A214 ERW Tubes – welded heat exchanger and condenser tubes
Frequently Asked Questions – ASTM A334 Grade 6 Tubes
What is ASTM A334 Grade 6?
ASTM A334 Grade 6 is a silicon-killed carbon-manganese steel grade for seamless and welded tubes intended for low-temperature service. It has a maximum of 0.30% carbon, 0.29–1.06% manganese and at least 0.10% silicon, a minimum tensile strength of 415 MPa and a minimum yield strength of 240 MPa, and it is Charpy impact tested at -45°C (-50°F).
What is the minimum design temperature for A334 Grade 6 tubes?
The standard Charpy impact test temperature for A334 Grade 6 is -45°C (-50°F). The minimum design metal temperature permitted in your system is set by the applicable design code (e.g. ASME B31.3 or ASME Section VIII), wall thickness and stress level – the test temperature alone does not fix it. For service below -45°C, nickel grades such as A334 Grade 7, 3 or 8 are used.
What is the difference between A334 Grade 6 and Grade 1?
Both are carbon steel grades impact tested at -45°C. Grade 6 requires a minimum of 0.10% silicon (fully killed) and has higher strength – 415 MPa tensile and 240 MPa yield versus 380 MPa and 205 MPa for Grade 1 – with a maximum hardness of B90 against B85 for Grade 1.
What is the difference between ASTM A334 Grade 6 and ASTM A333 Grade 6?
A334 covers tubes ordered by outside diameter and minimum wall thickness, typically for heat exchangers and small-bore lines. A333 covers pipe ordered by nominal pipe size and schedule with average wall thickness. The chemistry, tensile properties and -45°C impact requirement for Grade 6 are essentially the same in both specifications.
Is ASME SA334 Grade 6 the same as ASTM A334 Grade 6?
Yes, technically. ASME adopts the ASTM specification into the Boiler and Pressure Vessel Code as SA334. Tubes are commonly dual-certified as ASTM A334 / ASME SA334 Grade 6, which allows their use in ASME code-stamped equipment.
What is the hardness of A334 Grade 6 tubes?
The maximum hardness for A334 Grade 6 is Rockwell B90, equivalent to about 190 HB. For sour service under NACE MR0175, a lower hardness limit of 22 HRC applies to the finished tube and is easily met by normalized Grade 6.
Are A334 Grade 6 tubes available in seamless and welded form?
Yes. The specification covers both seamless and welded (without filler metal) tubes. Seamless tubes are preferred for high-pressure and critical heat-exchanger duty; welded tubes are an economical option for many standard applications.
Can A334 Grade 6 tubes be supplied as U-bend tubes?
Yes. We supply A334 Grade 6 U-bend tubes bent to customer drawings, with stress relieving of the bend area and hydrostatic testing after bending when specified.
Can A334 Grade 6 tubes be welded?
Yes. With carbon limited to 0.30% and a controlled manganese range, Grade 6 has good weldability. For low-temperature service, welding procedures should be qualified with impact testing at the design temperature, as required by ASME Section VIII and B31.3.
What certificates are supplied with A334 Grade 6 tubes?
Each supply includes an EN 10204 3.1 mill test certificate showing chemistry, mechanical, hardness, impact and hydro/NDE results. EN 10204 3.2 certification with third-party inspection by agencies such as TÜV, BV, SGS, Lloyd’s or DNV is available on request.