ASTM A423 Grade 1 Tubes | ASME SA423 Gr 1 Corten Steel APH Tubes Supplier

ASTM A423 Grade 1 tubes (ASME SA423 Gr 1) are seamless and electric-resistance welded (ERW) low-alloy steel tubes made for pressure parts that must resist corrosion – most commonly air preheater (APH) tubes and economizer tubes in boilers and power plants. ASC LLP, Mumbai, supplies A423 Gr 1 Corten steel tubes in hot-finished and cold-drawn condition, with EN 10204 3.1 mill certificates and IBR certification on request.

What Are ASTM A423 Grade 1 Tubes?

ASTM A423/A423M is the standard specification for seamless and electric-welded low-alloy steel tubes. It covers minimum-wall tubes for pressure-containing parts, such as economizers, and other applications where corrosion resistance is important. The usual size range is 1/2″ to 5″ (12.7 to 127 mm) OD with 0.035″ to 0.500″ (0.9 to 12.7 mm) minimum wall.

Grade 1 is a copper-chromium-nickel-phosphorus steel – the same alloying idea used in Corten steel (Corten A). These elements form a dense, adherent oxide layer that slows further attack. In flue-gas service, this gives A423 Gr 1 tubes better resistance than plain carbon steel to acid dew-point corrosion, which typically attacks the cold end of air preheaters and economizers. Grade 1 tubes have a minimum tensile strength of 415 MPa (60 ksi) and a minimum yield strength of 255 MPa (37 ksi).

Buyers also search for this product as:

  • ASME SA423 Grade 1 Tubes
  • A423 Gr 1 Corten Steel Tubes
  • Corten Steel APH Tubes (Air Preheater Tubes)
  • A423 Grade 1 ERW Tubes
  • A423 Grade 1 Seamless / Cold Drawn Tubes
  • Corten Economizer Tubes
ASTM A423 Grade 1 Corten steel tubes bundle for air preheaters

ASTM A423 Grade 1 Tubes Properties

Understanding the properties of A423 Gr 1 tubes shows why they are the standard choice for air preheaters and economizers:

  1. Corrosion Resistance: Copper, chromium, nickel and phosphorus build a protective oxide layer that resists atmospheric and flue-gas dew-point corrosion better than plain carbon steel tubes.
  2. Pressure Rating: Grade 1 tubes meet minimum tensile and yield strengths of 415 MPa and 255 MPa and are hydrostatically or NDE tested, so they are suitable for pressure-containing boiler parts.
  3. Formability: The specification requires tubes to be expanded and beaded into tube plates without cracking, which is essential for APH and economizer assembly.
  4. Controlled Hardness: Hardness is limited to 170 HBW / 87 HRBW, which keeps tubes soft enough for roller expansion.
  5. Weldability: With carbon limited to 0.15% max, Grade 1 tubes can be welded into headers and tube plates with qualified procedures.

Types of ASTM A423 Grade 1 Tubes We Supply

  • A423 Gr 1 Seamless Tubes – hot finished or cold drawn, for higher-pressure economizer coils
  • A423 Gr 1 ERW Tubes – electric-resistance welded, the most common form for air preheater tube banks
  • A423 Grade 1 APH Tubes – cut to length for tubular air preheaters, with plain or expanded ends
  • A423 Grade 1 Economizer Tubes – straight lengths and bends for economizer coils
  • IBR-Certified A423 Gr 1 Tubes – for boiler projects in India under the Indian Boiler Regulations

ASTM A423 Grade 1 Tubes Advantages

Choosing ASTM A423 Gr 1 tubes for your heat-recovery equipment offers several advantages:

  1. Longer Tube Life: Better resistance to dew-point corrosion at the cold end of air preheaters reduces tube leaks and replacement frequency.
  2. Lower Lifecycle Cost: Fewer tube failures and shutdowns usually outweigh the slightly higher cost compared with carbon steel tubes such as ASTM A214 or A178.
  3. Code Acceptance: As ASME SA423, Grade 1 is accepted for pressure parts under the ASME Boiler & Pressure Vessel Code.
  4. Seamless or ERW Choice: Buyers can choose ERW tubes for economy or seamless tubes for higher-pressure duty, both under the same specification.
  5. Easy Fabrication: Controlled hardness and formability make expansion, beading and welding into tube plates straightforward.
ASME SA423 Grade 1 ERW air preheater tubes with mill marking
ASTM A423 Grade 1 economizer tube coil for boilers

Size Chart for ASTM A423 Grade 1 Tubes

Outside Diameter (inch) Outside Diameter (mm) Minimum Wall Thickness Range (mm)
1/2″ 12.70 0.9 – 2.1
3/4″ 19.05 1.2 – 2.8
1″ 25.40 1.2 – 3.4
1-1/4″ 31.75 1.65 – 4.2
1-1/2″ 38.10 1.65 – 4.5
1-3/4″ 44.45 2.1 – 5.0
2″ 50.80 2.1 – 5.6
2-1/2″ 63.50 2.4 – 6.4
3″ 76.20 2.8 – 7.1
4″ 101.60 3.0 – 8.0
5″ 127.00 3.4 – 12.7

A423 tubes are ordered by outside diameter and minimum wall thickness. Common air preheater sizes are 38.1, 44.45, 50.8 and 63.5 mm OD. Other sizes are available on request.

Mechanical Properties of ASTM A423 Grade 1 Tubes

Property Requirement
Tensile Strength, min 60,000 psi (415 MPa)
Yield Strength, min 37,000 psi (255 MPa)
Elongation in 2″ (50 mm), min 25%
Hardness, max 170 HBW (Brinell) / 87 HRBW (Rockwell B)

Specifications Chart – ASTM A423 Grade 1 Tubes

Specification Description
Standard ASTM A423 / A423M, ASME SA423 / SA423M
Grade Grade 1 (Gr. 1) – Cu-Cr-Ni-P low-alloy (Corten type) steel
General Requirements ASTM A450 / A450M
Type Seamless, Electric-Resistance Welded (ERW)
Finish Hot finished, cold finished (cold drawn)
Outside Diameter 12.7 mm (1/2″) to 127 mm (5″) – other sizes on request
Wall Thickness 0.9 mm to 12.7 mm (minimum wall)
Length Single random, double random, cut lengths up to 12 m
Ends Plain end, bevelled end
Heat Treatment Normalized, or heat treated as needed to meet the specification
Surface Black, varnished, anti-rust oil
Test Certificate EN 10204 3.1 / 3.2, IBR (Form III) on request
Third-Party Inspection TÜV, BV, SGS, Lloyd’s, DNV, EIL or client inspector

Tensile Strength Chart – ASTM A423 Grades 1, 2 and 3

Property Grade 1 Grade 2 Grade 3
Tensile Strength, min 415 MPa (60 ksi) 415 MPa (60 ksi) 380 MPa (55 ksi)
Yield Strength, min 255 MPa (37 ksi) 255 MPa (37 ksi) 230 MPa (33 ksi)
Elongation in 2″ (50 mm), min 25% 25% 35%

For longitudinal strip tests, the minimum elongation is reduced by 1.25 percentage points for each 1/32″ (0.8 mm) decrease in wall thickness below 5/16″ (8 mm).

Minimum Elongation by Wall Thickness – A423 Grade 1 (Strip Specimens)

Wall Thickness Min. Elongation in 2″ (50 mm)
5/16″ (8 mm) and over 25%
9/32″ (7.2 mm) 24%
1/4″ (6.4 mm) 22.5%
7/32″ (5.6 mm) 21%
3/16″ (4.8 mm) 20%
5/32″ (4 mm) 19%
1/8″ (3.2 mm) 17.5%
3/32″ (2.4 mm) 16%
1/16″ (1.6 mm) 15%

Values are calculated from the specification’s 1.25-point deduction rule and rounded to the nearest 0.5%.

Heat Treatment Requirement Chart – ASTM A423 Grade 1

Condition Requirement
All tubes Normalized, or given the heat treatment needed to meet the specification’s mechanical requirements
Cold-drawn tubes Heat treated after the final cold-drawing pass
Welded (ERW) tubes Heat treated after welding, so the weld zone matches the base metal
Lot size – tubes 2″ OD and over, wall 0.200″ and over Not more than 50 tubes per heat-treatment lot
Lot size – tubes 1″ OD and under Not more than 125 tubes per heat-treatment lot

Testing & Quality Control of A423 Grade 1 Tubes

Every lot of ASTM A423 Grade 1 tubes is tested to the specification and ASTM A450, and the results are reported on the mill test certificate:

  • Heat and product chemical analysis
  • Tension test
  • Flattening test
  • Flaring test (seamless tubes)
  • Flange test and reverse flattening test (welded tubes)
  • Hardness test (Brinell / Rockwell)
  • Hydrostatic test or non-destructive electric test (eddy current / ultrasonic)
  • Expansion and beading capability as required for boiler tube insertion
  • Visual and dimensional inspection; PMI and third-party inspection on request

ASTM A423 Grade 1 vs Grade 2 vs Grade 3 – Chemical Composition

Element (%) Grade 1 Grade 2 Grade 3
Carbon, max 0.15 0.15 0.06
Manganese 0.55 max 0.50 – 1.00 0.70 – 1.40
Phosphorus 0.06 – 0.16 0.04 max 0.020 max
Sulfur, max 0.060 0.05 0.020
Silicon 0.10 min — 0.55 max
Copper 0.20 – 0.60 0.30 – 1.00 0.25 – 0.45
Chromium 0.24 – 1.31 — —
Nickel 0.20 – 0.70 0.40 – 1.10 0.50 max
Molybdenum — 0.10 min 0.20 max
Antimony — — 0.05 – 0.15

Which grade should you choose? Grade 1 is the Corten-type grade and the one most specified for air preheater tubes. Grade 2 is a copper-nickel-molybdenum steel with the same strength. Grade 3 is a low-carbon, antimony-bearing grade aimed at sulfuric-acid dew-point corrosion.

Physical Properties Chart – A423 Grade 1 (Typical)

Property Value
Density 7.85 g/cm³
Melting Range approx. 1420°C – 1510°C
Thermal Conductivity approx. 45 W/m·K (at 20°C)
Specific Heat approx. 0.47 J/g·K
Modulus of Elasticity approx. 200 GPa
Coefficient of Thermal Expansion approx. 12 × 10⁻⁶ /°C (20–100°C)

These are typical values for low-alloy steel, given for design reference. ASTM A423 does not specify physical properties.

Application Chart – ASTM A423 Grade 1 Tubes

Application Description
Air Preheaters (APH) Tubular air preheaters in boilers, where flue gas cools below its acid dew point at the cold end
Economizers Feedwater economizer coils that recover heat from boiler exhaust gas
Power Plants Coal, biomass and waste-heat recovery boilers
Sugar Mills & Distilleries Bagasse-fired boiler air preheaters
Cement & Steel Plants Waste-heat recovery and gas-to-air heat exchangers
Refineries & Petrochemicals Fired-heater air preheaters and flue-gas heat recovery
Paper, Chemical & Fertilizer Plants Process boilers and heat exchangers exposed to corrosive gases

ASTM A423 Grade 1 Equivalent Grades

Standard Equivalent / Comparable Grade
ASTM A423 Grade 1
ASME SA423 Grade 1
Trade Name Corten A type chemistry (Cu-Cr-Ni-P)
Comparable Plate / Sheet Grades ASTM A242 Type 1, ASTM A606 Type 4
Comparable EN Grade S355J2WP (EN 10025-5) – weathering steel

These grades share a similar weathering-steel chemistry but are not direct substitutes for pressure tubes. Confirm suitability against your design code before substituting.

Related Products

Why Choose ASC LLP as your ASME SA423 Gr 1 Tubes Supplier?

As a leading ASTM A423 Grade 1 tubes manufacturer and supplier, ASC LLP provides tubes that meet the specification and your project documentation requirements:

  1. Experience Since 1984: Decades of supplying carbon, alloy and Corten steel tubes to boiler makers, EPC contractors and plant owners.
  2. Mill-Sourced, Traceable Material: Tubes from approved mills, with heat numbers marked on every tube and matching EN 10204 3.1 / 3.2 certificates.
  3. IBR & Third-Party Inspection: IBR certification and inspection by TÜV, BV, SGS, Lloyd’s, DNV or EIL on request.
  4. Competitive Pricing: Direct mill tie-ups keep A423 Gr 1 tube prices competitive without compromising quality.
  5. Timely Delivery: Ready stock of common APH sizes and export-ready packing in bundles or wooden boxes.

Whether you are replacing an air preheater tube bank or building a new economizer, our ASTM A423 Grade 1 tubes deliver longer life in corrosive flue-gas service.

Frequently Asked Questions – ASTM A423 Grade 1 Tubes

What is ASTM A423 Grade 1?

ASTM A423 Grade 1 is a copper-chromium-nickel-phosphorus low-alloy steel grade for seamless and electric-welded tubes used in pressure parts where corrosion resistance matters, such as air preheaters and economizers. It has a minimum tensile strength of 415 MPa and a minimum yield strength of 255 MPa.

Is ASTM A423 Grade 1 the same as Corten steel?

A423 Grade 1 uses the same Cu-Cr-Ni-P alloying concept as Corten A weathering steel, which is why it is widely sold as Corten steel tube. However, A423 is a pressure-tube specification with its own tests, so buy to ASTM A423 / ASME SA423 when the tubes go into boiler pressure parts.

Why are A423 Grade 1 tubes used in air preheaters?

At the cold end of an air preheater, flue gas cools below its acid dew point and condenses corrosive acids onto the tubes. The alloying elements in Grade 1 slow this attack compared with plain carbon steel tubes, which extends tube life and reduces leaks.

What is the difference between A423 Grade 1, Grade 2 and Grade 3?

Grade 1 is a Cu-Cr-Ni-P (Corten-type) steel. Grade 2 is a Cu-Ni-Mo steel with the same 415/255 MPa strength. Grade 3 is a low-carbon, antimony-bearing grade with lower strength (380/230 MPa) and higher elongation, designed for sulfuric-acid dew-point corrosion.

Is ASME SA423 Grade 1 the same as ASTM A423 Grade 1?

Yes. ASME adopts ASTM A423 into the Boiler and Pressure Vessel Code as SA423. Tubes are usually dual-certified to ASTM A423 / ASME SA423 Grade 1.

What sizes do ASTM A423 Grade 1 tubes come in?

The specification usually covers 1/2″ to 5″ (12.7 to 127 mm) OD with 0.035″ to 0.500″ (0.9 to 12.7 mm) minimum wall thickness. Other sizes can be supplied if they meet all other requirements.

Are A423 Grade 1 tubes available seamless and welded?

Yes. The standard covers both seamless and electric-resistance welded tubes, in hot-finished or cold-finished condition. ERW tubes are most common for air preheaters; seamless tubes are often used for economizer coils.

What is the maximum hardness of A423 Grade 1 tubes?

The maximum hardness is 170 HBW (Brinell) or 87 HRBW (Rockwell B). This keeps the tubes soft enough to be expanded and beaded into tube plates without cracking.

Do you supply IBR-certified A423 Grade 1 tubes?

Yes. We can supply A423 Grade 1 tubes with IBR certification for boiler projects in India, along with EN 10204 3.1 or 3.2 certificates and third-party inspection.

Global Reach

Amardeep Steel Centre supplies clients around the world, with a reputation for prompt delivery and reliable documentation. Boiler makers, power producers and EPC companies across the USA, Europe, the Middle East and Asia trust our ASTM A423 Grade 1 tubes for air preheater and economizer projects.

Metal-globe

Countries We Export To

UNITED STATES, EUROPE, UK, UAE, SAUDI ARABIA, OMAN, KUWAIT, JORDAN, QATAR, INDONESIA, MALAYSIA, BRAZIL, SPAIN, ITALY, FRANCE, GERMANY, BAHRAIN, SRI LANKA, AZERBAIJAN, AUSTRALIA, AUSTRIA, PHILIPPINES, TURKEY, RUSSIA, IRAN, IRAQ, CANADA, KOREA, JAPAN, YEMEN, FINLAND, ZIMBABWE, HUNGARY, PORTUGAL, VIETNAM, MOROCCO, THAILAND, SOUTH AFRICA, MEXICO, SINGAPORE, GREECE, KUWAIT, POLAND, NEW ZEALAND, SWEDEN, SWITZERLAND, BELGIUM, BHUTAN, BANGLADESH, TAIWAN, ROMANIA, CAMBODIA, KAZAKHSTAN, AFGHANISTAN.

Follow us on: