ASC LLP, Mumbai, supplies ASME SA387 Grade 5 Class 1 plates (ASTM A387 Gr 5 Cl 1) in 6 mm to 150 mm thickness, sourced from approved mills and cut to size on request. In addition, every plate comes with an EN 10204 3.1 certificate. This page therefore covers the SA387 Grade 5 material in full, including chemical composition, Class 1 and Class 2 properties, heat treatment, welding and matching grades.
What is ASME SA387 Grade 5?
ASME SA387 / ASTM A387 is the specification for chromium-molybdenum alloy steel plates for pressure vessels, especially welded boilers and vessels for elevated-temperature service. Within it, Grade 5 (UNS K41545) is a 5% chromium – ½% molybdenum steel. As a result, it resists high-temperature oxidation as well as sulphur and hydrogen attack better than lower-chromium grades such as Grade 11 or Grade 22.
Each grade is supplied in two strength levels. Class 1 is the lower-strength level (415–585 MPa tensile), while Class 2 is the higher-strength level. Since the chemistry is the same for both classes, the class is set by the heat treatment. For this reason, always state the class on the order, for example “SA387 Gr 5 Cl 1”. For Class 2, see our SA387 Grade 5 Class 2 plates page.
SA387 Grade 5 Class 1 – Quick Facts
- Specification: ASME SA387 / ASTM A387, Grade 5 Class 1 (UNS K41545)
- Composition: 4.00–6.00% Cr, 0.45–0.65% Mo
- Class 1 strength: 415–585 MPa tensile / 205 MPa yield min
- Heat treatment: annealed, or normalised and tempered (temper 705 °C min)
- Thickness: 6 mm to 150 mm (others on request)

SA387 Grade 5 Chemical Composition
| Element | SA387 Grade 5 (%) |
| Carbon (C) | 0.15 max |
| Manganese (Mn) | 0.30 – 0.60 |
| Phosphorus (P) | 0.025 max |
| Sulphur (S) | 0.025 max |
| Silicon (Si) | 0.50 max |
| Chromium (Cr) | 4.00 – 6.00 |
| Molybdenum (Mo) | 0.45 – 0.65 |
These are heat analysis limits, so product analysis allows a small tolerance (for example Mn 0.25–0.66% and Cr 3.90–6.10%). In addition, the composition is the same for Class 1 and Class 2. Where better weldability is needed, buyers may also specify a restricted carbon content of 0.10% max.
SA387 Grade 5 Class 1 Mechanical Properties
| Property | Grade 5 Class 1 | Grade 5 Class 2 |
| Tensile strength | 415 – 585 MPa (60 – 85 ksi) | 515 – 690 MPa (75 – 100 ksi) |
| Yield strength, min | 205 MPa (30 ksi) | 310 MPa (45 ksi) |
| Elongation in 50 mm, min | 18% | 18% |
| Reduction of area, min (Class 1) | 45% round / 40% flat specimen | – |
Because Class 1 is tempered to a lower strength, it is more ductile and easier to form. Class 2, on the other hand, allows thinner shells for the same pressure. Therefore, the choice depends on the design code allowable stresses for your vessel.


SA387 Grade 5 Heat Treatment
- Permitted treatments: A387 Grade 5 plates are annealed, normalised and tempered, or accelerated-cooled and then tempered.
- Tempering temperature: at least 705 °C (1300 °F) for Grade 5, so the plate reaches a stable, tough structure.
- Simulated PWHT: in addition, buyers often order test coupons given a simulated post-weld heat treatment, because the vessel will be stress relieved after fabrication.
SA387 Grade 5 Class 1 Plate Specifications
| Item | Details |
| Specification | ASME SA387 / ASTM A387, Grade 5 Class 1 |
| Thickness | 6 mm to 150 mm; also thicker on request |
| Width / length | Up to 3000 mm wide and 12000 mm long, or cut to size |
| Condition | Annealed, or normalised and tempered |
| General requirements | ASTM A20 / ASME SA20 |
| Testing | Tensile and chemistry per heat; in addition, UT (A435 / A578), Charpy impact and simulated PWHT on request |
| Edges | Mill edge or gas cut; also bevelled to drawing |
| Certificate | EN 10204 3.1; also 3.2 and third-party inspection on request |
SA387 Grade 5 Plate Sizes
| Thickness (mm) | Common plate sizes (mm) |
| 6 – 12 | 1500 / 2000 / 2500 × 6000 / 8000 |
| 16 – 40 | 2000 / 2500 × 6000 / 8000 / 10000 |
| 50 – 100 | 2000 / 2500 × 6000 / 8000 |
| 100 – 150 | By mill enquiry; also cut pieces |
These are typical stock and mill sizes, so availability can vary by thickness. However, we can supply cut pieces, circles and rings to your drawing.
SA387 Grade 5 Equivalent & Matching Grades
| Product form | Matching 5Cr-½Mo grade |
| Plate (Class 2) | SA387 Grade 5 Class 2 |
| Seamless pipe | ASTM A335 P5 |
| Forged fittings | ASTM A182 F5 |
| Flanges | ASTM A182 F5 flanges |
| Tubes | ASTM A213 T5 |
| EN plate equivalent | EN 10028-2 X12CrMo5 (1.7362) |
Because these grades share the same 5Cr-½Mo chemistry, a vessel or piping system can be built from plate, pipe, fittings and flanges of one material family. However, an “equivalent” grade may differ in strength or testing, so check it against your design code.
Welding SA387 Grade 5 Plates
- P-number: SA387 Grade 5 is a P-No. 5B material, so it needs a qualified procedure with preheat and post-weld heat treatment.
- Preheat: typically around 200 °C, because 5Cr steels harden on cooling.
- Filler metal: matching 5Cr-½Mo consumables such as E8015-B6 / ER80S-B6.
- PWHT: usually about 705–760 °C; afterwards, hardness of weld and HAZ is often checked.
Applications of SA387 Grade 5 Class 1 Plates
| Industry | Typical SA387 Grade 5 use |
| Oil refining | Hydrotreater and heater equipment, because 5Cr resists sulphur and hydrogen attack |
| Petrochemical | High-temperature reactors, separators and drums |
| Heat exchangers | Shells, channels and tube sheets in Cr-Mo service |
| Furnaces & heaters | Tube supports and high-temperature components |
| Power & boilers | Pressure parts in elevated-temperature service |
Grade 5 is chosen for its high-temperature strength and resistance to sulphidation and hydrogen attack. However, it is not a stainless steel, so wet corrosive service still needs stainless or clad plate.
SA387 Grade 5 vs Grade 11, 22, 9 & 91
| Grade | Composition | Class 1 tensile / yield (MPa) | Typical use |
| Grade 11 | 1¼Cr – ½Mo – Si | 415–585 / 240 | Boilers and vessels up to about 550 °C |
| Grade 22 | 2¼Cr – 1Mo | 415–585 / 205 | Hydrogen service and vessels up to about 595 °C |
| Grade 5 | 5Cr – ½Mo | 415–585 / 205 | Sulphur and hydrogen service at high temperature |
| Grade 9 | 9Cr – 1Mo | 415–585 / 205 | More severe high-temperature sulphidation |
| Grade 91 | 9Cr – 1Mo – V – Nb | Class 2 only: 585–760 / 415 | Highest creep strength |
In short, chromium content rises from Grade 11 to Grade 9, and so does resistance to high-temperature sulphidation. See also our Grade 12 plates, the ASME SA387 alloy steel plates hub and our alloy steel products.
Frequently Asked Questions – SA387 Grade 5 Class 1 Plates
What is ASME SA387 Grade 5 Class 1?
SA387 Grade 5 Class 1 is a 5% chromium – ½% molybdenum alloy steel pressure vessel plate in the lower-strength class (415–585 MPa tensile). It is used for refinery and petrochemical vessels in high-temperature service.
What is the chemical composition of SA387 Grade 5?
SA387 Grade 5 contains C 0.15% max, Mn 0.30–0.60%, Si 0.50% max, Cr 4.00–6.00% and Mo 0.45–0.65%. In addition, P and S are each limited to 0.025% max.
What is the difference between SA387 Grade 5 Class 1 and Class 2?
Both have the same chemistry. However, Class 1 has 415–585 MPa tensile and 205 MPa yield, while Class 2 has 515–690 MPa tensile and 310 MPa yield.
Is SA387 Grade 5 normalized and tempered?
Yes, it is commonly normalised and tempered, although A387 also permits annealing or accelerated cooling and tempering. In every case, Grade 5 is tempered at 705 °C (1300 °F) minimum.
What is the equivalent of SA387 Grade 5?
The closest EN plate grade is X12CrMo5 (1.7362) to EN 10028-2. In addition, the matching product grades are A335 P5 pipe, A182 F5 forgings and A213 T5 tubes.
Is SA387 Grade 5 weldable?
Yes, but it needs care. Grade 5 is P-No. 5B, so it requires preheat, matching B6 filler metal and post-weld heat treatment.
Is SA387 Grade 5 corrosion resistant?
It resists high-temperature oxidation, sulphidation and hydrogen attack. However, it is not stainless steel, so it is not used for wet corrosive service.
Global Supply
ASC LLP supplies ASME SA387 Grade 5 Class 1 plates from Mumbai to customers in India, the Middle East, Europe, Africa, the Americas and South-East Asia. To get a prompt quotation, simply send your enquiry with thickness, size, class, testing and quantity.

Countries We Export To
UNITED STATES, EUROPE, UK, UAE, SAUDI ARABIA, OMAN, KUWAIT, JORDAN, QATAR, INDONESIA, MALAYSIA, BRAZIL, SPAIN, ITALY, FRANCE, GERMANY, BAHRAIN, SRI LANKA, AZERBAIJAN, AUSTRALIA, AUSTRIA, PHILIPPINES, TURKEY, RUSSIA, IRAN, IRAQ, CANADA, KOREA, JAPAN, YEMEN, FINLAND, ZIMBABWE, HUNGARY, PORTUGAL, VIETNAM, MOROCCO, THAILAND, SOUTH AFRICA, MEXICO, SINGAPORE, GREECE, KUWAIT, POLAND, NEW ZEALAND, SWEDEN, SWITZERLAND, BELGIUM, BHUTAN, BANGLADESH, TAIWAN, ROMANIA, CAMBODIA, KAZAKHSTAN, AFGHANISTAN.