ASTM A423 Grade 1 Tubes | ASME SA423 Gr 1 Corten Steel APH Tubes Supplier
ASTM A423 Grade 1 tubes (ASME SA423 Gr 1) are seamless and electric-resistance welded (ERW) low-alloy steel tubes made for pressure parts that must resist corrosion – most commonly air preheater (APH) tubes and economizer tubes in boilers and power plants. ASC LLP, Mumbai, supplies A423 Gr 1 Corten steel tubes in hot-finished and cold-drawn condition, with EN 10204 3.1 mill certificates and IBR certification on request.
What Are ASTM A423 Grade 1 Tubes?
ASTM A423/A423M is the standard specification for seamless and electric-welded low-alloy steel tubes. It covers minimum-wall tubes for pressure-containing parts, such as economizers, and other applications where corrosion resistance is important. The usual size range is 1/2″ to 5″ (12.7 to 127 mm) OD with 0.035″ to 0.500″ (0.9 to 12.7 mm) minimum wall.
Grade 1 is a copper-chromium-nickel-phosphorus steel – the same alloying idea used in Corten steel (Corten A). These elements form a dense, adherent oxide layer that slows further attack. In flue-gas service, this gives A423 Gr 1 tubes better resistance than plain carbon steel to acid dew-point corrosion, which typically attacks the cold end of air preheaters and economizers. Grade 1 tubes have a minimum tensile strength of 415 MPa (60 ksi) and a minimum yield strength of 255 MPa (37 ksi).
Buyers also search for this product as:
- ASME SA423 Grade 1 Tubes
- A423 Gr 1 Corten Steel Tubes
- Corten Steel APH Tubes (Air Preheater Tubes)
- A423 Grade 1 ERW Tubes
- A423 Grade 1 Seamless / Cold Drawn Tubes
- Corten Economizer Tubes

ASTM A423 Grade 1 Tubes Properties
Understanding the properties of A423 Gr 1 tubes shows why they are the standard choice for air preheaters and economizers:
- Corrosion Resistance: Copper, chromium, nickel and phosphorus build a protective oxide layer that resists atmospheric and flue-gas dew-point corrosion better than plain carbon steel tubes.
- Pressure Rating: Grade 1 tubes meet minimum tensile and yield strengths of 415 MPa and 255 MPa and are hydrostatically or NDE tested, so they are suitable for pressure-containing boiler parts.
- Formability: The specification requires tubes to be expanded and beaded into tube plates without cracking, which is essential for APH and economizer assembly.
- Controlled Hardness: Hardness is limited to 170 HBW / 87 HRBW, which keeps tubes soft enough for roller expansion.
- Weldability: With carbon limited to 0.15% max, Grade 1 tubes can be welded into headers and tube plates with qualified procedures.
Types of ASTM A423 Grade 1 Tubes We Supply
- A423 Gr 1 Seamless Tubes – hot finished or cold drawn, for higher-pressure economizer coils
- A423 Gr 1 ERW Tubes – electric-resistance welded, the most common form for air preheater tube banks
- A423 Grade 1 APH Tubes – cut to length for tubular air preheaters, with plain or expanded ends
- A423 Grade 1 Economizer Tubes – straight lengths and bends for economizer coils
- IBR-Certified A423 Gr 1 Tubes – for boiler projects in India under the Indian Boiler Regulations
ASTM A423 Grade 1 Tubes Advantages
Choosing ASTM A423 Gr 1 tubes for your heat-recovery equipment offers several advantages:
- Longer Tube Life: Better resistance to dew-point corrosion at the cold end of air preheaters reduces tube leaks and replacement frequency.
- Lower Lifecycle Cost: Fewer tube failures and shutdowns usually outweigh the slightly higher cost compared with carbon steel tubes such as ASTM A214 or A178.
- Code Acceptance: As ASME SA423, Grade 1 is accepted for pressure parts under the ASME Boiler & Pressure Vessel Code.
- Seamless or ERW Choice: Buyers can choose ERW tubes for economy or seamless tubes for higher-pressure duty, both under the same specification.
- Easy Fabrication: Controlled hardness and formability make expansion, beading and welding into tube plates straightforward.


Size Chart for ASTM A423 Grade 1 Tubes
| Outside Diameter (inch) | Outside Diameter (mm) | Minimum Wall Thickness Range (mm) |
| 1/2″ | 12.70 | 0.9 – 2.1 |
| 3/4″ | 19.05 | 1.2 – 2.8 |
| 1″ | 25.40 | 1.2 – 3.4 |
| 1-1/4″ | 31.75 | 1.65 – 4.2 |
| 1-1/2″ | 38.10 | 1.65 – 4.5 |
| 1-3/4″ | 44.45 | 2.1 – 5.0 |
| 2″ | 50.80 | 2.1 – 5.6 |
| 2-1/2″ | 63.50 | 2.4 – 6.4 |
| 3″ | 76.20 | 2.8 – 7.1 |
| 4″ | 101.60 | 3.0 – 8.0 |
| 5″ | 127.00 | 3.4 – 12.7 |
A423 tubes are ordered by outside diameter and minimum wall thickness. Common air preheater sizes are 38.1, 44.45, 50.8 and 63.5 mm OD. Other sizes are available on request.
Mechanical Properties of ASTM A423 Grade 1 Tubes
| Property | Requirement |
| Tensile Strength, min | 60,000 psi (415 MPa) |
| Yield Strength, min | 37,000 psi (255 MPa) |
| Elongation in 2″ (50 mm), min | 25% |
| Hardness, max | 170 HBW (Brinell) / 87 HRBW (Rockwell B) |
Specifications Chart – ASTM A423 Grade 1 Tubes
| Specification | Description |
| Standard | ASTM A423 / A423M, ASME SA423 / SA423M |
| Grade | Grade 1 (Gr. 1) – Cu-Cr-Ni-P low-alloy (Corten type) steel |
| General Requirements | ASTM A450 / A450M |
| Type | Seamless, Electric-Resistance Welded (ERW) |
| Finish | Hot finished, cold finished (cold drawn) |
| Outside Diameter | 12.7 mm (1/2″) to 127 mm (5″) – other sizes on request |
| Wall Thickness | 0.9 mm to 12.7 mm (minimum wall) |
| Length | Single random, double random, cut lengths up to 12 m |
| Ends | Plain end, bevelled end |
| Heat Treatment | Normalized, or heat treated as needed to meet the specification |
| Surface | Black, varnished, anti-rust oil |
| Test Certificate | EN 10204 3.1 / 3.2, IBR (Form III) on request |
| Third-Party Inspection | TÜV, BV, SGS, Lloyd’s, DNV, EIL or client inspector |
Tensile Strength Chart – ASTM A423 Grades 1, 2 and 3
| Property | Grade 1 | Grade 2 | Grade 3 |
| Tensile Strength, min | 415 MPa (60 ksi) | 415 MPa (60 ksi) | 380 MPa (55 ksi) |
| Yield Strength, min | 255 MPa (37 ksi) | 255 MPa (37 ksi) | 230 MPa (33 ksi) |
| Elongation in 2″ (50 mm), min | 25% | 25% | 35% |
For longitudinal strip tests, the minimum elongation is reduced by 1.25 percentage points for each 1/32″ (0.8 mm) decrease in wall thickness below 5/16″ (8 mm).
Minimum Elongation by Wall Thickness – A423 Grade 1 (Strip Specimens)
| Wall Thickness | Min. Elongation in 2″ (50 mm) |
| 5/16″ (8 mm) and over | 25% |
| 9/32″ (7.2 mm) | 24% |
| 1/4″ (6.4 mm) | 22.5% |
| 7/32″ (5.6 mm) | 21% |
| 3/16″ (4.8 mm) | 20% |
| 5/32″ (4 mm) | 19% |
| 1/8″ (3.2 mm) | 17.5% |
| 3/32″ (2.4 mm) | 16% |
| 1/16″ (1.6 mm) | 15% |
Values are calculated from the specification’s 1.25-point deduction rule and rounded to the nearest 0.5%.
Heat Treatment Requirement Chart – ASTM A423 Grade 1
| Condition | Requirement |
| All tubes | Normalized, or given the heat treatment needed to meet the specification’s mechanical requirements |
| Cold-drawn tubes | Heat treated after the final cold-drawing pass |
| Welded (ERW) tubes | Heat treated after welding, so the weld zone matches the base metal |
| Lot size – tubes 2″ OD and over, wall 0.200″ and over | Not more than 50 tubes per heat-treatment lot |
| Lot size – tubes 1″ OD and under | Not more than 125 tubes per heat-treatment lot |
Testing & Quality Control of A423 Grade 1 Tubes
Every lot of ASTM A423 Grade 1 tubes is tested to the specification and ASTM A450, and the results are reported on the mill test certificate:
- Heat and product chemical analysis
- Tension test
- Flattening test
- Flaring test (seamless tubes)
- Flange test and reverse flattening test (welded tubes)
- Hardness test (Brinell / Rockwell)
- Hydrostatic test or non-destructive electric test (eddy current / ultrasonic)
- Expansion and beading capability as required for boiler tube insertion
- Visual and dimensional inspection; PMI and third-party inspection on request
ASTM A423 Grade 1 vs Grade 2 vs Grade 3 – Chemical Composition
| Element (%) | Grade 1 | Grade 2 | Grade 3 |
| Carbon, max | 0.15 | 0.15 | 0.06 |
| Manganese | 0.55 max | 0.50 – 1.00 | 0.70 – 1.40 |
| Phosphorus | 0.06 – 0.16 | 0.04 max | 0.020 max |
| Sulfur, max | 0.060 | 0.05 | 0.020 |
| Silicon | 0.10 min | — | 0.55 max |
| Copper | 0.20 – 0.60 | 0.30 – 1.00 | 0.25 – 0.45 |
| Chromium | 0.24 – 1.31 | — | — |
| Nickel | 0.20 – 0.70 | 0.40 – 1.10 | 0.50 max |
| Molybdenum | — | 0.10 min | 0.20 max |
| Antimony | — | — | 0.05 – 0.15 |
Which grade should you choose? Grade 1 is the Corten-type grade and the one most specified for air preheater tubes. Grade 2 is a copper-nickel-molybdenum steel with the same strength. Grade 3 is a low-carbon, antimony-bearing grade aimed at sulfuric-acid dew-point corrosion.
Physical Properties Chart – A423 Grade 1 (Typical)
| Property | Value |
| Density | 7.85 g/cm³ |
| Melting Range | approx. 1420°C – 1510°C |
| Thermal Conductivity | approx. 45 W/m·K (at 20°C) |
| Specific Heat | approx. 0.47 J/g·K |
| Modulus of Elasticity | approx. 200 GPa |
| Coefficient of Thermal Expansion | approx. 12 × 10⁻⁶ /°C (20–100°C) |
These are typical values for low-alloy steel, given for design reference. ASTM A423 does not specify physical properties.
Application Chart – ASTM A423 Grade 1 Tubes
| Application | Description |
| Air Preheaters (APH) | Tubular air preheaters in boilers, where flue gas cools below its acid dew point at the cold end |
| Economizers | Feedwater economizer coils that recover heat from boiler exhaust gas |
| Power Plants | Coal, biomass and waste-heat recovery boilers |
| Sugar Mills & Distilleries | Bagasse-fired boiler air preheaters |
| Cement & Steel Plants | Waste-heat recovery and gas-to-air heat exchangers |
| Refineries & Petrochemicals | Fired-heater air preheaters and flue-gas heat recovery |
| Paper, Chemical & Fertilizer Plants | Process boilers and heat exchangers exposed to corrosive gases |
ASTM A423 Grade 1 Equivalent Grades
| Standard | Equivalent / Comparable Grade |
| ASTM | A423 Grade 1 |
| ASME | SA423 Grade 1 |
| Trade Name | Corten A type chemistry (Cu-Cr-Ni-P) |
| Comparable Plate / Sheet Grades | ASTM A242 Type 1, ASTM A606 Type 4 |
| Comparable EN Grade | S355J2WP (EN 10025-5) – weathering steel |
These grades share a similar weathering-steel chemistry but are not direct substitutes for pressure tubes. Confirm suitability against your design code before substituting.
Related Products
- ASTM A847 Tubes – Corten square, rectangular and round structural tubing
- Corten Steel Seamless Pipes – round weathering steel pipes
- ASTM A334 Grade 6 Tubes – low temperature carbon steel heat exchanger tubes
Why Choose ASC LLP as your ASME SA423 Gr 1 Tubes Supplier?
As a leading ASTM A423 Grade 1 tubes manufacturer and supplier, ASC LLP provides tubes that meet the specification and your project documentation requirements:
- Experience Since 1984: Decades of supplying carbon, alloy and Corten steel tubes to boiler makers, EPC contractors and plant owners.
- Mill-Sourced, Traceable Material: Tubes from approved mills, with heat numbers marked on every tube and matching EN 10204 3.1 / 3.2 certificates.
- IBR & Third-Party Inspection: IBR certification and inspection by TÜV, BV, SGS, Lloyd’s, DNV or EIL on request.
- Competitive Pricing: Direct mill tie-ups keep A423 Gr 1 tube prices competitive without compromising quality.
- Timely Delivery: Ready stock of common APH sizes and export-ready packing in bundles or wooden boxes.
Whether you are replacing an air preheater tube bank or building a new economizer, our ASTM A423 Grade 1 tubes deliver longer life in corrosive flue-gas service.
Frequently Asked Questions – ASTM A423 Grade 1 Tubes
What is ASTM A423 Grade 1?
ASTM A423 Grade 1 is a copper-chromium-nickel-phosphorus low-alloy steel grade for seamless and electric-welded tubes used in pressure parts where corrosion resistance matters, such as air preheaters and economizers. It has a minimum tensile strength of 415 MPa and a minimum yield strength of 255 MPa.
Is ASTM A423 Grade 1 the same as Corten steel?
A423 Grade 1 uses the same Cu-Cr-Ni-P alloying concept as Corten A weathering steel, which is why it is widely sold as Corten steel tube. However, A423 is a pressure-tube specification with its own tests, so buy to ASTM A423 / ASME SA423 when the tubes go into boiler pressure parts.
Why are A423 Grade 1 tubes used in air preheaters?
At the cold end of an air preheater, flue gas cools below its acid dew point and condenses corrosive acids onto the tubes. The alloying elements in Grade 1 slow this attack compared with plain carbon steel tubes, which extends tube life and reduces leaks.
What is the difference between A423 Grade 1, Grade 2 and Grade 3?
Grade 1 is a Cu-Cr-Ni-P (Corten-type) steel. Grade 2 is a Cu-Ni-Mo steel with the same 415/255 MPa strength. Grade 3 is a low-carbon, antimony-bearing grade with lower strength (380/230 MPa) and higher elongation, designed for sulfuric-acid dew-point corrosion.
Is ASME SA423 Grade 1 the same as ASTM A423 Grade 1?
Yes. ASME adopts ASTM A423 into the Boiler and Pressure Vessel Code as SA423. Tubes are usually dual-certified to ASTM A423 / ASME SA423 Grade 1.
What sizes do ASTM A423 Grade 1 tubes come in?
The specification usually covers 1/2″ to 5″ (12.7 to 127 mm) OD with 0.035″ to 0.500″ (0.9 to 12.7 mm) minimum wall thickness. Other sizes can be supplied if they meet all other requirements.
Are A423 Grade 1 tubes available seamless and welded?
Yes. The standard covers both seamless and electric-resistance welded tubes, in hot-finished or cold-finished condition. ERW tubes are most common for air preheaters; seamless tubes are often used for economizer coils.
What is the maximum hardness of A423 Grade 1 tubes?
The maximum hardness is 170 HBW (Brinell) or 87 HRBW (Rockwell B). This keeps the tubes soft enough to be expanded and beaded into tube plates without cracking.
Do you supply IBR-certified A423 Grade 1 tubes?
Yes. We can supply A423 Grade 1 tubes with IBR certification for boiler projects in India, along with EN 10204 3.1 or 3.2 certificates and third-party inspection.
Global Reach
Amardeep Steel Centre supplies clients around the world, with a reputation for prompt delivery and reliable documentation. Boiler makers, power producers and EPC companies across the USA, Europe, the Middle East and Asia trust our ASTM A423 Grade 1 tubes for air preheater and economizer projects.

Countries We Export To
UNITED STATES, EUROPE, UK, UAE, SAUDI ARABIA, OMAN, KUWAIT, JORDAN, QATAR, INDONESIA, MALAYSIA, BRAZIL, SPAIN, ITALY, FRANCE, GERMANY, BAHRAIN, SRI LANKA, AZERBAIJAN, AUSTRALIA, AUSTRIA, PHILIPPINES, TURKEY, RUSSIA, IRAN, IRAQ, CANADA, KOREA, JAPAN, YEMEN, FINLAND, ZIMBABWE, HUNGARY, PORTUGAL, VIETNAM, MOROCCO, THAILAND, SOUTH AFRICA, MEXICO, SINGAPORE, GREECE, KUWAIT, POLAND, NEW ZEALAND, SWEDEN, SWITZERLAND, BELGIUM, BHUTAN, BANGLADESH, TAIWAN, ROMANIA, CAMBODIA, KAZAKHSTAN, AFGHANISTAN.